Dielectric Strength Approx. |
N/A 500 V/mil |
Thermal Conductivity (Average) |
N/A 4.4 x 10-4 x (cal·cm/ºC·cm·s) 1.3 BTU i./h·ft2 ºF |
Specific Heat |
N/A 0.3 BTU/lb/ºF |
Linear Thermal Expansion1 | N/A 1.5 x 10-4 |
Width/Sheet Size |
N/A 36 in |
Color |
N/A Gray |
Thickness2 | N/A 1/16 ±.005 in1/32 ±.005 in1/8 ±.010 in3/32 ±.010 in |
ZZ-R-765, Class 3b (Grade) |
N/A 70 |
AMS |
N/A 3349 |
Test Method Durometer |
N/A D2240 |
Durometer (Shore A ±5)3 | N/A 70 |
Test Method Tensile Strength |
N/A D412 |
Tensile Strength4 | N/A 1200 psi |
Test Method Elongation |
N/A D412 |
Elongation5 | N/A 350 % |
Test Method Tear Strength |
N/A D624 |
Tear Strength6 | N/A 150 ppi |
Test Method Compression Set |
N/A D395 |
Compression Set after 70 h at 320 ºF7 | N/A 30 % |
Durometer Change (Points, Shore A) after Dry Heat Aging for 70 h at 437 ºF |
N/A +10 |
Tensile Strength Change after Dry Heat Aging for 70 h at 437 ºF |
N/A –25 % |
Elongation Change after Dry Heat Aging for 70 h at 437 ºF |
N/A –35 % |
Durometer Change (Points, Shore A) after Immersion in ASTM Oil #1 (High Aniline Point) for 70 H at 302 ºF |
N/A –5 |
Tensile Strength Change after Immersion in ASTM Oil #1 (High Aniline Point) for 70 H at 302 ºF |
N/A 0 % |
Elongation Change after Immersion in ASTM Oil #1 (High Aniline Point) for 70 H at 302 ºF |
N/A –5 % |
Volume Change after Immersion in ASTM Oil #1 (High Aniline Point) for 70 H at 302 ºF |
N/A +5 % |