Dielectric Strength Approx.
|
|
500 V/mil
|
|
Thermal Conductivity (Average)
|
|
4.4 x 10-4 x (cal·cm/ºC·cm·s) 1.3 BTU i./h·ft2 ºF
|
|
Specific Heat
|
|
0.3 BTU/lb/ºF
|
|
Linear Thermal Expansion1
|
|
1.5 x 10-4
|
|
Width/Sheet Size
|
|
36 in
|
|
Color
|
|
Red
|
|
Thickness2
|
|
1/16 ±.005 in 1/32 ±.005 in 1/8 ±.010 in 3/32 ±.010 in
|
|
ZZ-R-765, Class 2a & 2b (Grade)
|
|
50
|
|
AMS
|
|
3302
|
|
Test Method Durometer
|
|
D2240
|
|
Durometer (Shore A ±5)3
|
|
50
|
|
Test Method Tensile Strength
|
|
D412
|
|
Tensile Strength4
|
|
900 psi
|
|
Test Method Elongation
|
|
D412
|
|
Elongation5
|
|
400 %
|
|
Test Method Tear Strength
|
|
D624
|
|
Tear Strength6
|
|
75 ppi
|
|
Test Method Compression Set
|
|
D395
|
|
Compression Set after 70 h at 320 ºF7
|
|
15 %
|
|
Durometer Change (Points, Shore A) after Dry Heat Aging for 70 h at 437 ºF
|
|
+5
|
|
Tensile Strength Change after Dry Heat Aging for 70 h at 437 ºF
|
|
–10 %
|
|
Elongation Change after Dry Heat Aging for 70 h at 437 ºF
|
|
–30 %
|
|
Durometer Change (Points, Shore A) after Immersion in ASTM Oil #1
(High Aniline Point) for 70 H at 302 ºF
|
|
–10
|
|
Tensile Strength Change after Immersion in ASTM Oil #1
(High Aniline Point) for 70 H at 302 ºF
|
|
–10 %
|
|
Elongation Change after Immersion in ASTM Oil #1
(High Aniline Point) for 70 H at 302 ºF
|
|
–5 %
|
|
Volume Change after Immersion in ASTM Oil #1
(High Aniline Point) for 70 H at 302 ºF
|
|
+5 %
|
|
1 Room temperature to +350 ºF
2 Thickness 3/32 in - special order. Minimum quantities apply.
3 Die B Method B, ASTM D2000 + Fed. Spec. ZZ-R-765.
4 Die B Method B, ASTM D2000 + Fed. Spec. ZZ-R-765.
5 Die B Method B, ASTM D2000 + Fed. Spec. ZZ-R-765.